Mainly are out of
tolerance, corrugated, fluffed, blistered and uneven surface, etc.
(1) The
out-of-tolerance pipe diameter is mainly because the resin content of the
prepreg is too high or exceeds the standard, the soluble resin content is too
low, and the melting degree is poor during rolling, which is exposed on the reinforcing
material surface.
(2) The resin
content and soluble resin content of the corrugated prepreg are too large or
exceed the index value, the molding time of the epoxy adhesive is too long, and
the glue accumulates during rolling to form corrugation, bubbling, and even
cracking.
(3) The reasons
for layering and layering are mainly: the material in the aging section of the
prepreg is not removed, and the prepreg with low resin content and soluble
resin value is rolled into the blank of the laminated tube; or the prepreg
Insufficient arc segments wrapped on the hot roller, coupled with the fact that
the ventilation system above the rolling machine is not activated or the air
volume is insufficient, it is difficult to remove volatiles.
(4) The surface of the tube is fluffy and not smooth. Before dipping the paint, the inner and outer surfaces of the laminated tube should be trimmed to make them smooth; at the same time, the impregnating paint used should be filtered in time to remove impurities; the impregnating material frame should be regularly removed. Subs and paint clots.